Microstructure And Properties Of Ti-3Al-5Mo-4.5V Titanium Alloy For Cold Heading Fasteners

Ti-3Al-5Mo-4.5V titanium alloy (BT16) was developed by the Russian Light Alloy Research Institute. It is a high-strength, new and typical α+β two-phase titanium alloy. It has excellent mechanical properties and cold heading forming. The alloy's The main semi-finished products are rolled and drawn wires and bars with a diameter of 4 to 10 mm. Aviation fasteners such as screws, bolts and rivets can be made through cold heading.
The characteristics of BT16 titanium alloy are as follows: it contains a small amount of Al, more beta stabilizing elements (Mo), the beta phase stability coefficient Kβ is as high as 0.8, the beta phase content is about 25% to 30%, and it has high stability in the annealed or quenched state. Plasticity, while solid solution + aging alloys have higher strength, but the plasticity does not decrease significantly. The main transition phases that appear in titanium alloys during heat treatment are α′ phase, α″ phase and quenching aging β phase.
Russia uses annealed BT16 alloy wire for cold heading to make aviation fasteners. Domestic and foreign scholars have conducted extensive research on the annealing process, microstructure, phase structure and mechanical properties of BT16 titanium alloy. Cold deformation strengthened fasteners made of BT16 alloy have the lowest labor hours and costs, and can be used indefinitely below 160°C; fasteners made of solid solution aging BT16 alloy can operate at temperatures up to 350°C.
In order to provide theoretical basis and experimental data for further research and optimization of BT16 titanium alloy and its applications, researchers studied the evolution of the organizational structure of BT16 titanium alloy during the production process by using optical microscope (OM), scanning electron microscope (SEM) and transmission electron microscope (TEM). And the influence of heat treatment process on the mechanical properties of alloy wire.
In the experiment, BT16 titanium alloy wire with a diameter of 6.5mm was used, and its chemical composition is shown in Table 1. The preparation process of alloy wire is as follows: ingot casting → blanking → forging → rolling. First, two vacuum consumable electrode melting furnaces are used to obtain a Φ210mm BT16 titanium alloy ingot, and then the billet is opened. The starting temperature is 1150°C, the end temperature is controlled at about 800°C, and then hot forged into a wire with a diameter of 7.5mm. , and finally annealing treatment: 780°C for 2 hours, furnace cooling to 550°C, and then air cooling. The surface of the annealed wire is polished to prepare for cold heading experiments.

news-620-163

BT16 titanium alloy wire and cold heading samples were observed using LEICA DM2500M upright transmission and reflection optical microscope (OM), JEOL JEM?2100 transmission electron microscope (TEM) and JEOL JSEM?7001F high-resolution scanning electron microscope (SEM). and analysis. The chemical corrosive ratio is 2.5mLHf+3mLHNO3+5mLHCl+89.5mLH2O. The test results are as follows:
(1) The annealing system of BT16 alloy wire is: 760~830℃, 2h+550℃, air cooling. The mechanical properties of the obtained wire are σb of 870 to 935 MPa, δ of 22% to 25%, and ψ of 62% to 65%. Its cold heading deformation reaches 80%. After annealing, the alloy structure consists of primary equiaxed α phase, a small amount of It consists of short strip α phase and intergranular β phase.
(2) After solid solution (air cooling) + aging, the alloy structure consists of irregular equiaxed primary α phase and β phase with precipitated needle-like α′ phase; after solid solution (quenching) + aging, the alloy consists of equiaxed α phase. A two-state structure composed of primary α phase and intergranular β phase, which is composed of primary α phase, intergranular β phase and needle-like α′ phase precipitated within β phase.